Mapping and release of chemical substances from products made of chloroprene
Table 4.4 Results of x-ray analysis (weight percentage)
Sample/Brand |
Mg |
Al |
Si |
Cl |
S |
Ca |
Ti |
Fe |
Zn |
Ni |
Cr |
Dive gloves /3 |
0.053 |
0.67 |
0.74 |
0.0053 |
0.85 |
5.7 |
0.033 |
0.035 |
0.60 |
< 0.003 |
< 0.003 |
3 (surface, inside) |
0.0045 |
0.0010 |
0.0021 |
0.52 |
0.097 |
0.67 |
0.036 |
0.008 |
0.17 |
< 0.003 |
0.0067 |
Dive gloves /7 |
0.19 |
1.7 |
2.5 |
0.028 |
0.98 |
1.8 |
0.072 |
0.14 |
0.81 |
< 0.003 |
< 0.003 |
7 (surface, inside) |
0.023 |
0.043 |
0.075 |
0.88 |
0.15 |
0.26 |
0.13 |
0.037 |
0.27 |
< 0.003 |
0.0087 |
No other elements were detected.
Detection limit: 0.003%.
The results for the surfaces includes an unknown amount of the contents of the rubber itself as the surface layer (fabric) is thin.